Solution: The problem of sticking nodules in the deep drawing process of stainless steel sheet has always plagued the production site, bringing great trouble to the producers. However, because the formation of sticking nodules involves tribology and other issues, there are many influencing factors. At present, we can only propose measures from different angles to prevent and reduce the formation of adhesion nodules.
Material selection and heat treatment of the working part of the mold: For the problem of adhesion, the selection of the mold material should be based on the affinity between the stainless steel sheet and the mold material. Pay attention to two points: the first choice is strong anti-adhesion, and the second is wear resistance and friction reduction mold material.
Generally speaking, metals with the same lattice type, lattice spacing, electron density, and electrochemical properties are attracted to each other, have strong solubility, and are easy to stick together, resulting in a larger friction coefficient. The mutual solubility of Cr, Ni and Fe is large, so when deep drawing with steel die, the phenomenon of sticking nodules is more likely to occur. Practice has proved that the anti-stick effect of cast aluminum bronze and hard aluminum bronze is better; the use of tungsten carbide steel bonded cemented carbide to manufacture the die is several times higher than that of Cr12Mov soft nitriding to manufacture the die, and the die does not stick; if the code is used For 3054 alloy cast iron, only flame quenching is required on the surface of the mold, and there will be no adhesion nodules on the surface of the mold.
In addition, cemented carbide inserts can be used in the vulnerable parts of the mold, which has excellent compressive performance, superior wear resistance and durable surface roughness and dimensional accuracy control.But due to price issues, it is less used in production. Restricted by the material selection of the factory, if general high-carbon and high-chromium tool steel is used as a stainless steel sheet drawing die, the heat treatment hardness should reach 60HRC or more, and the surface can be nitrocarburized. If the hardness is increased in order to improve the wear resistance of the die, the bonding phenomenon in the deep drawing of stainless steel will not be improved. The key is that the retained austenite should be removed as much as possible during the heat treatment.
For high-hardness materials such as Cr12, a common quenching process is used. Even if the ultimate hardness range of HRC62-64 is reached, a considerable amount of austenite remains in the structure. Austenite is not only the soft spot in the mold, but also has a weaker affinity with the active agent in the lubricant than martensite, so it is not easy to establish a lubricating oil film. Therefore, the heat treatment of such materials can be treated at low temperature after quenching and cooling, so that the retained austenite is transformed into martensite to improve the adhesion resistance of the matrix. In addition, the stainless steel deep drawing die should be surface treated to improve the wear resistance and adhesion resistance of the die. For molds made of alloy cast iron or non-ferrous alloy materials, surface strengthening processes such as nitriding are used, and the effect is better.
2. Surface processing of the working part of the mold requires high surface quality of the stainless steel deep drawing die. Lower surface roughness can reduce friction and improve adhesion resistance. Therefore, after the drawing die has been ground, it is more important to eliminate machining marks. In mold manufacturing, the grinding and polishing processes are often ignored. It should be pointed out that in the entire mold processing process, the polishing workload should account for one-third, because the appearance quality of stainless steel products depends to a large extent on the polishing of the mold. grinding technique.
The surface roughness of the mold is reduced, the grinding times of the mold is correspondingly reduced, and the service life of the mold is correspondingly improved. If the surface of the mold is not polished enough, and the deep drawing of the stainless steel sheet is easy to cause the characteristics of adhesion nodules, the products drawn from the deep drawing have serious scratches. These scratches on the product are time-consuming and ineffective to solve with polishing treatment. Therefore, we should put a lot of effort into the mold polishing process. Only by improving the surface processing accuracy of the mold can we reduce the scratches of the product and greatly improve the mold repair life of the mold.
In recent years, various new polishing technologies and polishing tools have appeared in China, and new processes and new equipment such as ultrasonic wave, electrolytic polishing, abrasive jet, and extrusion grinding have been developed. According to the data, the electrochemical polishing experiment was carried out on the molds of CrWMo, 3Cr12W8V and Cr12, and it was proved that this polishing can make the surface roughness of the mold cavity from the original Ra3.2-Ra1.6 in only 5-10 minutes. On the basis of reducing to Ra0.4-Ra0.2.
At the same time, the surface hardness can be improved by electrochemical polishing to improve the wear resistance. For another example, an ultrasonic polishing machine can be used for fine polishing of nitrocarburized cavities, which can avoid the disadvantage of easily destroying the nitride film by manual polishing. We should actively use and summarize the new polishing technology. 3. Process lubrication: From the deep drawing characteristics of stainless steel, it can be seen that the formation of the adhesion tumor is due to the direct contact between the sheet metal and the die. The lubricating film does not break and plays a lubricating role throughout the material stretching process.
"Anti-viscosity and friction reduction" is the basic starting point for selecting lubricants. Generally, adding a certain proportion of extreme pressure additives to the lubricant or using solid lubricants can achieve better results. This is mainly to improve the lubricating ability of the lubricant to the metal surface, to generate compounds containing sulfur, phosphorus and chlorine to chemically react with the metal surface at high temperature to generate iron sulfide, iron chloride, etc. to strengthen the oil film strength and enhance the adsorption capacity , Better lubrication of mold and product surface.
The solid lubricant is filled into the small pits on the metal surface to minimize the dry friction contact points. In addition, the solid lubricant has high stability and can also play a lubricating role at high temperatures, and it is not easy to cause mold bonding. Usually in production according to the degree of deformation of the product and the actual situation to select and formula (the formula can be found in the relevant stamping manual). In addition, the lubricant can also be composed of fat, mineral oil, synthetic grease, lubricating grease and soap liquid, and the effect of shallow drawing of stainless steel is better. Organo-mineral oils containing water-soluble emulsions or diluted with oil can also be used for shallow drawing.
Adding graphite to the lubricant can play an anti-adhesion effect, but it is more difficult to clean after graphite is added. If you choose 3054 alloy cast iron to make the mold, then the general lubricant will be better. According to the data, a layer of metal soft mold (such as copper, zinc, lead, etc.) can be obtained on the surface of the sheet after salt bath treatment, and the phenomenon of mold sticking will not occur during the deep drawing process. In addition, in recent years, an organic polymer lubricating film with polyvinyl butyral as the main body has been developed. After the blank is treated, a layer of organic lubricating film is obtained on the surface, which can be deformed together with the sheet, which not only avoids the mold The direct contact with the sheet material prevents sticking and ensures the surface quality of the product. Moreover, the friction between the mold and the sheet metal is greatly weakened, and it plays a good lubricating effect. The experiment shows that the effect is good.